    The cause and solution of crack in casting aluminum alloy

    Release Time:2023-02-13      Number of clicks:143

    The cause and solution of crack in casting aluminum alloy


    Casting aluminum alloy Aluminum alloy, aluminum alloy castings can be obtained directly from parts by the metal casting process. The alloying element content of these alloys is generally higher than that of the corresponding deformed aluminum alloys.


    The content of alloyed element silicon in cast aluminum alloy is larger than that in most deformed aluminum alloys. In addition to the reinforcement element, the cast aluminum alloy must contain a sufficient amount of eutectic element (usually silicon) so that the alloy has considerable fluidity and is easy to fill the shrinkage joint of the casting.


    Casting crack is a crack formed at a higher temperature in the volume shrinkage of large alloy and more complex shape of the casting prone to appear.


    Cause:


    1. The structure design of castings is not reasonable, with sharp corners and the wall thickness changes are too different


    2. Sand mold (core) is not conciliatory


    3. Local overheating of the casting mold


    4. The pouring temperature is too high


    5. Premature removal of castings from the casting mold


    6. Heat treatment overheating or overburning, cooling speed is excessive


    Solution:


    1. Improve the structural design of castings, avoid sharp corners, and strive for uniform wall thickness and smooth transition


    2. Take measures to increase the yield of sand mold (core)


    3. Ensure that all parts of the casting are solidified simultaneously or sequentially, and improve the design of the pouring system


    4. Properly reduce pouring temperature


    5. Control the cold drawing time of the mold


    6. Hot calibration is adopted when casting is deformed


    7. Correctly control the heat treatment temperature to reduce the quenching cooling speed


    Previous:A brief discussion on casting quality inspection and defect repair
    Next:NO!

    Return list

    NEWS YOU MAY BE INTERESTED IN

    亚洲aⅴ天堂av天堂无码麻豆 | 久久综合伊人| 女人18片毛片60分钟| 中文精品无码中文字幕无码专区| 漂亮人妻被中出中文字幕| 99久久国产综合精品成人影院| 波多野结衣AV无码中文无码| 强行18分钟处破痛哭av| 免费无遮挡无码永久视频 | 中文字幕一区二区三区久久网站| 亚洲av无码久久| 无码人妻精品中文字幕| 久久综合狠狠色综合伊人| 曰韩无码无遮挡a级毛片| 日韩av无码久久精品免费| 精品成在人线av无码免费看| 人人妻人人澡人人爽精品日本 | 无码人妻丰满熟妇区五十路| 日本xxxx色视频在线播放| 亚洲日韩精品欧美一区二区一| 一区二区三区国产亚洲网站| 乱亲女h秽乱长久久久| 亚洲最大无码中文字幕| 亚洲精品乱码久久久久久蜜桃| 中国老太婆bb无套内射| 日韩综合网站| 久久蜜桃亚洲一区二区| 97精品人妻一区二区三区香蕉| 午夜无码一区二区三区在线观看| 亚洲欧美不卡高清在线观看| 国产美女亚洲精品久久久综合 | 亚洲AV优女天堂熟女| 无码国模国产在线观看| 中文字幕久无码免费久久| 亚洲va久久久噜噜噜久久狠狠 | 99久re热视频这里只有精品6| 亚洲av午夜福利精品一区| 欧美老熟妇喷水| 成人精品一区二区三区电影| 我把护士日出了白浆| 亚洲一区二区三区影院|